FCNS03 Fe Cu Ni Sn Pre Alloyed Powder don Ceramic Diamond Blade
FCNS03 Fe Cu Ni Sn Pre Alloyed Powder don Ceramic Diamond Blade
1. Menene Pre-alloyed Powder
Foda da aka riga aka yi amfani da su sun fi wuya, ba su da ƙarfi don haka suna buƙatar manyan matsi don samar da ƙaƙƙarfan ƙima.Duk da haka, suna iya samar da babban ƙarfi sintered kayan.Ana kuma amfani da riga-kafi a lokacin da samar da wani abu mai kama da juna daga foda na asali yana buƙatar yanayin zafi sosai da kuma tsawon lokaci mai tsayi.Mafi kyawun misalan su ne bakin ƙarfe, wanda abubuwan da ke cikin chromium da nickel dole ne a riga an haɗa su don ba da damar samar da tattalin arziki ta hanyar ƙarfe na foda.
2. Ma'auni naFarashin FCNS03
Babban Abun | Fe, Ku, Ni, Sn | |
Yawan Ka'idar | 7.98g/cm³ | |
Tsananin Zazzabi | 830 ℃ | |
Karfin Lankwasawa | 1150Mpa | |
Tauri | 104-108HRB |
3. FCNS03 Hali
- Tsarin Sintered ya kasance iri ɗaya ne kuma ƙarami.gawa yana da iko mai kyau na lu'u-lu'u, juriya mai girma da kaifi.
- Ana amfani da foda zuwa matsakaici zuwa babban ingancin dutsen lu'u-lu'u, yankan yumbu.
4. Umarni don Yin yumbu Yankan Ruwa.
- Karfe Kashi:
- (30-50)% FCNS03
- + (25-35)% Ku
- + (5-8)% Sn
- + (2-4)% Ni
- + Fe don Blance
B. Girman Gishiri na Diamond da Kashi:
- 50/60 @ 30%
- 60/70 @ 40%
- 70/80 @ 30%
- Hankali: (9-12)%
C. Yawan zafin jiki: 840-860 ℃